丁基胶出丝不断才叫涂得匀
时间:2026-11-27 来源:https://www.jncsjx.com/ 发布人:昌盛机械
中空玻璃一道密封靠的就是丁基胶这条“内封边”。外头有二道聚硫或硅酮挡水挡气,里头这层丁基胶才是真正管露点、管寿命、管氩气不漏的。现场翻车往往不是胶不好,是涂布机温度、胶嘴、铝条三样没对上——胶温低了出丝断、温高了流挂、铝条带水直接脱粘,合完片看着挺漂亮,放半年露点就飘。
The sealing of insulated glass relies on the "inner sealing edge" of butyl rubber. There are two layers of polysulfide or silicone water and gas barriers on the outside, and the layer of butyl rubber inside is the true dew point, lifespan, and argon gas leak proof layer of the pipe. On site overturning is often not due to poor adhesive quality, but rather a mismatch between the temperature of the coating machine, the nozzle, and the aluminum strip - the wire breakage occurs when the adhesive temperature is low, the sagging occurs when the temperature is high, and the aluminum strip directly detaches with water. After the film is closed, it looks beautiful, but after half a year, the dew point floats.
温度先按胶的“施工窗口”定,不按感觉
The temperature should be set according to the "construction window" of the adhesive first, not according to the feeling
丁基热熔胶常见施工温度 120–160℃,具体看厂家胶型:
The common construction temperature for butyl hot melt adhesive is 120-160 ℃, depending on the manufacturer's adhesive type:

普通丁基:130–145℃ 出丝顺;
Ordinary butyl: Straight silk at 130-145 ℃;
高粘度/低迁移款:150–165℃;
High viscosity/low migration version: 150-165 ℃;
温度低于 120℃:胶发硬、拉丝断、边角缺胶;
Temperature below 120 ℃: glue hardening, wire breakage, and missing glue at edges and corners;
超过 170℃:胶稀流挂,铝条立起来就往下淌,合片后溢到二道胶界面,反而脱粘。
Exceeding 170 ℃: The adhesive runs thin and hangs, causing the aluminum strip to stand up and flow downwards. After lamination, it overflows to the interface of the second layer of adhesive and instead becomes detached.
胶锅、胶管、胶嘴三段独立控温,温差超 ±5℃ 就容易时好时坏。冬天车间低于 10℃,胶锅预热要延长 20–30 分钟,别开机就涂。
The three-stage independent temperature control of the glue pot, rubber hose, and glue nozzle can easily fluctuate when the temperature difference exceeds ± 5 ℃. In winter, if the temperature in the workshop is below 10 ℃, the preheating of the glue pot should be extended by 20-30 minutes. Do not apply it immediately after turning on the machine.
胶嘴与铝条间隙,比泵压更关键
The gap between the nozzle and the aluminum strip is more critical than pump pressure
胶嘴出胶口一般 3–5mm,涂布厚度 0.8–1.2mm、宽度比铝条宽 0.5–1mm 为宜;
The glue nozzle usually has a glue outlet of 3-5mm, with a coating thickness of 0.8-1.2mm and a width 0.5-1mm wider than the aluminum strip;
胶嘴离铝条面 0.3–0.5mm,太近刮胶、太远拉丝拖尾;
The rubber nozzle is 0.3-0.5mm away from the aluminum strip surface, too close for scraping and too far for drawing and trailing;
铝条槽口建议干燥无油无粉尘,分子筛灌完到涂胶间隔别超 4 小时,返潮就擦净再过机;
The slot of the aluminum strip must be dry, oil-free, and dust-free. After filling the molecular sieve to the glue coating room, it should be separated by more than 4 hours. If it returns to moisture, it should be wiped clean before passing through the machine;
折弯铝角部位降速 30%,不然尖角堆胶、内角缺胶,二道封完也补不回来。
Reduce the speed of the bent aluminum corner by 30%, otherwise the sharp corners will accumulate glue and the inner corners will lack glue, and even after the second sealing, it will not be able to be replenished.
涂完到合片,时间窗卡死
After coating, the time window freezes when it comes to laminating
丁基胶是热熔压敏,表面结皮后就不粘了:
Butyl adhesive is a hot melt pressure-sensitive adhesive that does not stick after the surface has formed a skin
常温车间:涂完 ≤10 分钟进合片机;
Room temperature workshop: After coating, it takes ≤ 10 minutes to enter the laminating machine;
冬季或空调风直吹:≤5 分钟;
Winter or direct air conditioning blowing: ≤ 5 minutes;
超时铝框回锅重涂,别硬合。
Over time, the aluminum frame should be recoated and repainted. Do not forcefully close it.
很多线体“清洗—涂丁基—合片”三段节拍没配平,中间堆料十几分钟,露点测试一查就废。
Many production lines have an unbalanced three-stage cycle of "cleaning, butyl coating, and laminating", with materials piled up for more than ten minutes in the middle. Dew point testing results in waste.
设备日常三查,比换胶管用
Three daily checks on equipment, compared to replacing rubber hoses
胶锅残胶:连续停机 4 小时以上要降温保温,别让胶在锅里过夜碳化,碳化黑点就是日后针孔;
Residual glue in the glue pot: If the machine is stopped continuously for more than 4 hours, it should be cooled and kept warm. Do not let the glue carbonize overnight in the pot, as carbonization black spots will be pinholes in the future;
胶嘴清理:每班收工用铜刷+少量矿物油清嘴,禁火烧(烧嘴口变形出胶就歪);
Cleaning of nozzle: Use a copper brush and a small amount of mineral oil to clean the nozzle at the end of each shift. Do not burn it on fire (if the nozzle is deformed and produces glue, it will be crooked);
铝条导向轮:沾胶后带胶压进下一根铝条背面,整批污染,每 2 小时擦一次导向轮。
Aluminum strip guide wheel: After gluing, press the adhesive onto the back of the next aluminum strip, and the entire batch will be contaminated. Wipe the guide wheel every 2 hours.
验收盯四样
Acceptance inspection focuses on four samples
涂胶连续性:整圈无断点、无气泡、无堆胶角;
Continuity of glue application: no breakpoints, no bubbles, and no glue stacking angles throughout the entire circle;
截面测量:厚 0.8–1.2mm、宽覆盖铝条槽口全宽;
Cross section measurement: 0.8-1.2mm thick, covering the full width of the aluminum strip slot;
露点抽检:合片后按 GB/T 11944 测,−40℃ 无结露为合格线(Low-E 充气片更严);
Dew point sampling: After lamination, measure according to GB/T 11944, and the qualified line is -40 ℃ without condensation (Low-E inflatable sheet is stricter);
拉丝试验:胶温稳定后出丝应连续不断,断丝即温度或胶型不匹配。
Wire drawing test: After the glue temperature stabilizes, the wire should be continuously produced, and wire breakage is due to temperature or glue type mismatch.
丁基胶涂布机不是“加热挤出”那么简单,它是温度窗口 + 胶嘴间隙 + 铝条洁净 + 合片节拍四件事同时成立才出好活。前面糊弄,后面二道胶再贵也救不回露点。
The butyl rubber coating machine is not as simple as "heating extrusion". It requires the simultaneous establishment of four factors: temperature window, nozzle gap, aluminum strip cleanliness, and laminating rhythm to produce good results. No matter how expensive the second layer of glue is, it won't be able to save the exposed point.
本文由丁基胶涂布机友情奉献.更多有关的知识请点击:http://www.jncsjx.com我们将会对你提出的疑问进行详细的解答,欢迎你登录网站留言.
This article is a friendly contribution from the butyl rubber coating machine For more information, please click: http://www.jncsjx.com We will provide detailed answers to your questions. You are welcome to log in to our website and leave a message
- 丁基胶出丝不断才叫涂得匀 2026/11/27
- 停机那几分钟非常毁胶 2026/11/26
- 小片玻璃,卧式更顺手 2026/11/24
- 断胶先查温度 2026/11/20
- 胶温一飘,全框白涂 2026/11/18
- 折弯先看回弹量 2026/11/16
- 封胶线先看转角 2026/11/14
- 灌分子筛的隐形时钟 2026/11/12
- 一条线跑顺,先别只盯“全自动”三个字 2026/11/09
- 涂得准却压不上,卡在工序接缝那几秒 2026/11/06

当前位置: